Ukuthintela iziphene ezingabonakaliyo nge-PCB Lamination
Isiqulatho
- I-Blind Via PCB Lamination: Inkqubo yoKwakha ngokulandelelana vs. Inkqubo yoMjikelo omnye
- Iimfuneko zoMjikelo woKugalela iLamination ngohlobo lweHDI
- Ukulungiselela Ngaphambi Kokugalela Ilamination: Iimfuno Zeleya Yangaphakathi Nezinto Ezifunekayo
- Umjikelo wePress yeLamination: Iiparameter, iiPhase, kunye noLawulo lweNkqubo
- Ukucubungula iiBhayisikile eziPhakathi: Ukuhlolwa, ukuBhoboza, kunye nokuPlata phakathi kweeBhayisikile
- Iziphene eziqhelekileyo zeLamination, Izizathu ezisisiseko, kunye noThintelo
- Inkqubo ye-Highleap eLawulwayo ye-Lamination yee-HDI PCBs
I-Blind Via PCB Sequential Lamination — Iinkcukacha zeNkqubo eziphambili
- I-PCB esemgangathweni: Umjikelo we-lamination o-1 (zonke iileya zicinezelwe ngaxeshanye)
- Chwetheza I: Umaleko omnye wokwakheka kwe-microvia kumacala omabini okanye kwelinye, ngaphandle kwee-vias ezingcwatyiweyo; misela indlela yokwenyani yokucinezela.
- Uhlobo II: Umaleko omnye wokwakha ii-microvia one-vaas ezingcwatyiweyo; awufani nee-layers ezimbini zokwakha icala ngalinye.
- Uhlobo III: Iileya ezimbini okanye ngaphezulu zokwakheka kwe-microvia; bala imisebenzi ukusuka kulwakhiwo lokwenyani.
- Ixesha lomjikelo ngamnye: Landela iprofayili yoshicilelo eqinisekisiweyo ngezinto ezithile, kubandakanya ukufudumala, ukupholisa kunye nokupholisa.
- Imfuneko yobhaliso: ±0.075mm umaleko ukuya kumaleko (xa kuthelekiswa ne-±0.15mm i-PCB eqhelekileyo)
Indlela yokulaminatha eyimfama nge-PCB ixhomekeke kulandelelwano olukhutshiweyo lwe-stackup kunye nolwe-connection. Ulwakhiwo olulandelelanayo longeza kwaye luqhubekeke iileya ngamanqanaba ukuze kwenziwe unxibelelwano olungenakufikeleleka. Uhlobo lwe-HDI luchonga udidi lolwakhiwo; alugunyazisi inani elibanzi lemijikelo yokucinezela, iiyure ngomjikelo ngamnye okanye i-lead-time multiplier. Bala imisebenzi yoqobo, ulwakhiwo, ukubhola, i-plating kunye nokuhlolwa xa uphonononga iindleko kunye neshedyuli.
Cela ukwenziwa kwe-HDI nge-Lamination eLawulwayo
1. I-Blind Via PCB Lamination: Inkqubo yoKwakha ngokulandelelana vs. Inkqubo yoMjikelo omnye
1.1 Kutheni i-Standard Lamination ingenakuvelisa ii-Blind Vias
Kwimveliso yePCB esemgangathweni eneziteya ezininzi, zonke iileya zicinezelwa kunye kumjikelo omnye we-lamination. Emva kwe-lamination, ii-vias ezisebenzisa imingxunya zigqojozwa ngoomatshini ukusuka phezulu ukuya ezantsi, zidlula kuzo zonke iileya. Oku kuyasebenza kuba ii-vias ezisebenzisa imingxunya ziyafikeleleka kuzo zombini iibhodi.
Ii-vias ezingaboniyo, ngokwenkcazo, ziphela kumaleko athile angaphakathi kwaye azingeni kubukhulu bebhodi epheleleyo. Azinakwenziwa emva kokuba zonke iileya zifakwe i-laminate kuba:
- Ukubhola ngoomatshini akunakuma ngokuthembekileyo kubukhulu obuchanekileyo be-dielectric obuhambelana nomaleko othile wangaphakathi ngaphandle komngcipheko wokubhola ngokugqithisileyo.
- Ukubhola nge-laser (okunokufikelela kubunzulu obulawulwayo) akunamandla aneleyo okungena kwiileya ezingaphezu kwe-1-2 ze-FR-4 prepreg ngokupasa kube kanye
- Iphedi yobhedu engaphakathi ekufuneka i-blind ifike kuyo ifikeleleka kuphela ngaphambi kokuba iileya ezingaphezulu kwayo zifakwe i-laminate
I-lamination elandelelanayo isombulula oku ngokwakha umaleko webhodi ngokulandelelana: i-laminate ingaphakathi le-core, emva koko i-drill kwaye ifake i-blind vias kwi-buildup layer yokuqala ngaphambi kokongeza elandelayo.
1.2 Ulwakhiwo olulandelelanayo vs. I-Single Lamination: Uthelekiso lweNkqubo
| ukwakhiwa | Isiseko soqhagamshelwano | Uhlolo lwemijikelo kunye neshedyuli |
|---|---|---|
| I-multilayer eqhelekileyo | Ngokusebenzisa uqhagamshelo kwi-core/stackup echaziweyo. | Qinisekisa indlela yokucinezela kunye nokugrumba ebhodini; izakhiwo ezikhethekileyo zingongeza imisebenzi. |
| Chwetheza I HDI | Umaleko omnye wokwakheka kwe-microvia kumacala omabini okanye kwelinye; akukho zi-vias zingcwatyiweyo. | Bala imisebenzi engundoqo neyakhayo evunyiweyo; akukho mthetho wemijikelo emibini jikelele. |
| Uhlobo lwe-II HDI | Umaleko omnye wokwakheka kwe-microvia one-vias ezingcwatyiweyo kwisakhiwo. | Bandakanya imisebenzi yokuhlanganisa izinto ezingaphantsi komhlaba. |
| Uhlobo lwe-III HDI | Ubuncinane iileya ezimbini ze-microvia eziqokelelweyo kwicala elinye okanye omabini. | Hlaziya ulandelelwano lwe-layer-pair, ukuzalisa, ukuplata kunye nokuhlola inqanaba ngalinye. |
1.3 Kutheni uMjikelo ngamnye weLamination eyongezelelweyo udibanisa iindleko kunye nomngcipheko
Umjikelo ngamnye we-lamination wongeza:
- Iindleko ezithe ngqo: Ixesha lokushicilelwa, izinto zokulungiselela, ixesha lokuhlamba ngepleyiti — malunga ne-$18–$45/ibhodi ngobungakanani beprototype
- Ukuqokelelana kweempazamo zobhaliso: Umjikelo ngamnye uzisa ukungaqiniseki kobhaliso okungu-±0.025–0.075mm. Emva kwemijikelo emi-4, ukungaqiniseki okuqokelelweyo kunokufikelela ku-±0.10–0.15mm — kusondela kwinkcazo yeringi ejikelezayo ye-HDI enoxinano oluphezulu.
- Umngcipheko wesivuno: Umjikelo ngamnye unethuba eliyi-1–3% lokusilela kwenkqubo (ukwahlulahlula, ukungabi nanto, impazamo yokubhalisa) efuna ukuba iphaneli isuswe. Kwimijikelo emi-4, amathuba okuba umjikelo omnye ungasebenzi afikelela kwi-4–12%
- Ukuvezwa kubushushu: Umjikelo ngamnye we-lamination ubeka iileya ezigqityiweyo ngaphambili kwenye i-170–190°C. Izinto ezinobuthathaka kwi-Tg zinokubona utshintsho lwe-Dk. Izinto ezisekwe kwi-PTFE zifuna ulawulo lobushushu olucokisekileyo ngakumbi
Amanqanaba okwakha awongezelelweyo anokunyusa iindleko zenkqubo, ukuphathwa kunye nomngcipheko wesivuno. Isiphumo sixhomekeke kwisiseko esithile, i-microvia geometry, i-plating, izinto kunye nomthamo wemveliso; isiphindaphindi sexabiso esimiselweyo se-Type III-to-standard-board asinakuqondwa kwileyibhile ye-HDI yodwa.
2. Iimfuneko zoMjikelo woKugquma ngokohlobo lwe-HDI
2.1 Uhlobo I HDI Lamination Sequence
Uhlobo I lusebenzisa umaleko omnye wokwakha i-microvia kumacala omabini okanye kumacala omabini e-core, kunye ne-microvias ezingaboniyo kunye noqhagamshelwano oludlulayo kodwa akukho zi-vias ezifihliweyo. Umzekelo olinganayo ngu-1+N+1.
Umjikelo 1 — Ukufakwa kwe-Core lamination:
- Igalelo: Ii-cores zomaleko wangaphakathi ezinemifanekiso nezikroliweyo (L2 ukuya ku-L(n-1)), zilungelelaniswe phakathi kwee-cores, zincinci ifoyile yobhedu kwiindawo ezingaphandle
- Isiphumo: Umbindi wangaphakathi oqinisiweyo ngokupheleleyo kunye nomphezulu wangaphandle wobhedu oqinileyo (ezi ziya kuba yi-L2 kunye ne-L(n-1) emva kokulungiswa kwangaphandle)
- Uhlolo: Ukulinganiswa kobukhulu, ubhaliso lwe-X-ray, ukujonga ukususwa kombala emehlweni
Umjikelo 2 — Ukwakheka kwe-lamination yangaphandle:
- Igalelo: I-Core evela kwi-Cycle 1 (ene-blind via drilling, desmear, kunye ne-electroless copper phakathi kwemijikelo), i-laser-drillable prepreg, i-copper yangaphandle ebhityileyo (ngesiqhelo i-12–18µm foil)
- Isiphumo: Gqibezela isitaki esinee-multilayer kunye nazo zonke ii-layers ezibotshelelweyo
- Emva koMjikelo 2: Umzobo womaleko wangaphandle, ukukrola, imaski yesolder, ukugqitywa komphezulu, uvavanyo
2.2 Umzekelo we-Two-Buildup Lamination (Uhlobo lwesithathu)
Uhlobo lwesibini lukwasebenzisa umaleko omnye wokwakha i-microvia kumacala omabini okanye kumacala omabini ombindi, kwaye luquka ii-vas ezifihliweyo kunye nee-microvias ezingaboniyo kunye noqhagamshelwano oluhambayo. Akufanele ichazwe njenge-2+N+2.
Ukulungiswa komongo ongumzekelo: Lungisa umongo ovunyiweyo, kuquka naluphi na uqhagamshelo olufunekayo, ngaphambi kokuba kubekho ukwakheka kwee-microvia ezimbini.
Umjikelo 2 — Ulwakhiwo lokuqala lwangaphandle:
- I-laser-drill prepreg ebekwe embindini
- Emva kwalo mjikelo: Ukudlula kokuqala kwe-laser drill (ii-vias ezingaboniyo ukusuka kwi-L2 ukuya embindini), i-desmear, i-electroless copper, i-electroplating
- Kwi-microvias ezipakishiweyo: chaza ukuzaliswa kobhedu olufanelekileyo kunye nokulungiswa komphezulu okufunekayo ngaphambi kokwakhiwa okulandelayo.
- Kwi-staggered microvias: qinisekisa ukuba i-geometry isafuna ukuzaliswa okanye ukulungiswa okunye; ungacingi ukuba loo misebenzi iyanyamalala.
Umjikelo 3 — Ulwakhiwo lwesibini lwangaphandle:
- Isixhobo sesibini esinokwembiwa nge-laser esibekwe phezu kwesakhiwo seCycle 2
- Emva kwalo mjikelo: I-laser drill pass yesibini (ii-blind vias ukusuka kwi-L1 ukuya kwi-L2 pad), i-desmear, i-electroless, i-plating
- Emva koko ukucubungula umaleko wangaphandle kuyaqala
2.3 Uhlobo lwe-III HDI kunye ne-Core Buried Via Processing
Uhlobo lwesithathu lusebenzisa ubuncinane iileya ezimbini ze-microvia buildup kumacala omabini okanye kumacala omabini e-core kwaye lungabandakanya isakhiwo se-core esifunekayo esingcwatywe nge-braai. Umhambi wemveliso kufuneka achonge iileya zokwenyani kunye nolandelelwano lokucubungula :
Umjikelo ongaphantsi komongo 1 — L4–L5 ungcwatywe ngendlela yokwakheka:
- I-core laminate (iileya ze-L4–L5 kuphela) yombiwa ngoomatshini kwaye igqunywe ngeplastiki ukuze igqunywe ngeebhareli.
- I-L4 kunye ne-L5 zinemifanekiso egqunywe ngee-pads kunye nemikhondo edibanisayo
- I-sub-assembly engundoqo ihlolwe kwaye i-oxidized
Umjikelo ongaphantsi komongo 2 — I-lamination epheleleyo yomongo:
- I-sub-assembly ye-L4–L5, ii-cores ezisele zomaleko wangaphakathi, kunye ne-prepreg zidityaniswa kunye
- Ii-vias ezingcwatyiweyo ngoku zivaliwe ngokusisigxina ngaphakathi embindini
Imijikelo yokwakha yangaphandle efunekayo kwisakhiwo esikhutshiweyo: Ifakwe phezu kombindi opheleleyo.
Iimfuneko zokungcwaba zinokongeza imisebenzi yokubhola, ukuplata kunye nokulamina. Inani lemijikelo eyongeziweyo lixhomekeke ekubeni zeziphi iipaya zomaleko ezinokucutshungulwa kunye kunye nolwakhiwo oluvunyiweyo; ayisiyo ngokuzenzekelayo umjikelo omnye owongezelelweyo kwisibini ngasinye esikhankanyiweyo.
3. Ukulungiselela Ngaphambi Kokugalela Ilamination: Iimfuno Zeleya Yangaphakathi Nezinto Ezifunekayo
3.1 Iimfuneko zoMgangatho woMaleko wangaphakathi
Isiphumo ngasinye somjikelo we-lamination sixhomekeke kumgangatho wokwenziwa kweleya yangaphakathi yangaphambili:
Ukucoceka komphezulu wekopolo: Naluphi na ungcoliseko oluphilayo (ioyile, iminwe, intsalela ye-photoresist) kwikopolo yangaphakathi ithintela ukunamathela kwe-resin. Imiphezulu yekopolo icocwa ngenkqubo yamanyathelo amaninzi: i-alkaline cleaner, i-micro-etch (ukususwa kobhedu oluyi-1–2µm), ukuhlamba nge-asidi, ukuhlamba ngamanzi acocekileyo. Ucoceko luqinisekiswa ngovavanyo lokuqhekeka kwamanzi - umphezulu ocociweyo ngokufanelekileyo ubonisa ukumanzisa ngokulinganayo; ungcoliseko lubangela ukuqhekeka.
Unyango lwe-okside: Ubhedu olungenanto lunamandla aphantsi omphezulu kwaye alunamatheli kakuhle kwi-epoxy resin. Unyango lwe-oxide emdaka okanye i-oxide emnyama luyenza ibe rhabaxa umphezulu wobhedu ukusuka kwi-0.3–0.5µm (njengoko ikroliwe) ukuya kwi-1.5–3.0µm, nto leyo ephucula kakhulu amandla okukhupha amaxolo. Iinkqubo zanamhlanje "ze-micro-etch" okanye "zokukhuthaza ukunamathela kwendalo" (umz., iMacDermid MultiBond, iAtotech Universal Etch) zinokuthatha indawo ye-oxide kwiinkqubo ezithile ze-resin, kodwa kufuneka zifaneleke kwi-chemistry ethile ye-prepreg.
Ukuchaneka kobhaliso: Iithagethi zomaleko wangaphakathi (ngokuqhelekileyo iimpawu zobhedu ezimile okwe-cross-shaped) kufuneka zibe ngaphakathi kwe-±0.075mm ukusuka kwiindawo zazo eziqhelekileyo kwiinkqubo zokubhola ezilandelayo ukuze kugcinwe indandatho ye-annular. Iileya ezingaphandle kolu nyamezelano ziyasuswa ngaphambi kokulamination — kungekhona emva koko.
3.2 Ukulungiselela kunye nokulungiselela isicwangciso sokukhulelwa kwangaphambili
I-Prepreg (ilaphu le-fiberglass elifakwe i-B-stage epoxy resin ephiliswe kancinci) yinto yokubopha phakathi kweengqimba zobhedu. Iimfuneko ze-pre-lamination:
Ulawulo lokufuma: I-Prepreg ifunxa umswakama ovela emoyeni ongqongileyo. Ukufuma okungaphezulu kwe-0.2% kubangela oku:
- Ukuveliswa komphunga ngexesha lokulamina, okudala imingxuma kunye namadyungudyungu
- I-Tg encitshisiweyo ye-laminate ephilisiweyo
- Ukususwa kwe-delamination kwi-interface ye-copper-resin ngexesha lokucubungula ubushushu okulandelayo
Gcina kwaye uphathe i-prepreg ngokweemfuno zomthengisi wezinto ezisetyenzisiweyo, umswakama, ixesha elihlala ixesha elide kunye neemfuno zokulungiselela. I-Prepreg yinto engakaphiliswa: musa ukunika umthengisi i-120°C, ukubhaka iiyure ezimbini okunokutshintsha ukuhamba kwe-resin okanye ukuphiliswa kwangaphambili. Cela umthengisi ukuba alahle izinto ezisetyenzisiweyo ngembali yokugcina engaqinisekanga.
Ukukhetha kwangaphambili iileya zokwakheka ezinokugqojozwa nge-laser: Iileya zokwakheka zangaphandle ze-blind via formation kufuneka zigqojozwe nge-laser ngaphandle kwe-carbonization eya kungcolisa ngeendonga. I-standard luck fiberglass cloth prepreg kunzima ukuyigqobhoza nge-laser ngendlela ecocekileyo; ii-non-woven okanye modified glass-lap prepregs ezine-fiberglass content encitshisiweyo (umz., Panasonic R-1661W, Isola I-Tera MT40 prepreg, i-specialty low-loss laminate a specialty low-loss laminate bondply) zichaziwe kwiileya zokwakheka apho kucwangciswa khona ukugqobhozwa nge-laser (jonga ukugqobhozwa nge-laser ukuze ufumane i-microvia formation )
3.3 Ukukhethwa kweFoyile yeCopper kwiLayers zeBuildup
Iileya zangaphandle eziqokelelweyo zihlala zisebenzisa i-copper foil ebhityileyo (9–18µm) kune-inner cores (17–35µm).
- Ivumela isisombululo esicokisekileyo somfanekiso (umgama we-2/2 mil trace/space vs. 3/3 mil ubuncinci kwi-foil etyebileyo)
- Inciphisa ubungakanani bobhedu ekufuneka i-laser ibususe ngaphambi kokuba ifikelele kwi-prepreg, iphucula umgangatho wodonga.
- Ifuna ukuphathwa ngononophelo ukuze kuthintelwe ukushwabana ngexesha lokulamina
Kwiindlela zoyilo ezisebenzisa i-LP (Low Profile) okanye i-VLP (Very Low Profile) copper ukunciphisa ilahleko yokufaka i-high-frequency, ezi foils zisetyenziswa kuphela kwiileya zangaphandle zesignali apho i-frequency yesignali iqinisekisa iprimiyamu yexabiso. Iileya zangaphakathi ze-core zingasebenzisa i-ED copper eqhelekileyo.
4. Umjikelo wePress weLamination: Iiparameter, iiPhase, kunye noLawulo lweNkqubo
Iileya zangaphakathi, i-prepreg, kunye ne-copper foil zifakwe kwincwadi yokushicilela. Uxinzelelo loqhagamshelwano (50–100 PSI) lusetyenziswa ngaphambi kokufudumeza ukuthintela ukutshintsha kweleya ngexesha lokuhamba.
Ubushushu bokucinezela bunyuka kwi-2–4°C/min ukuya kwi-175–185°C. I-ramp ecothayo ivumela ukufuma komswakama kunye nokuhamba kwe-resin efanayo ngaphambi kokuba kuqale i-gelation.
Uxinzelelo olupheleleyo lwe-lamination (300–400 PSI) lufakiwe. I-resin iyahamba, izalisa izithuba, kunye nee-cross-links. Ubude bumiselwe yi-resin chemistry - ayinakufinyezwa.
Ubushushu buncitshisiwe kwi-2–4°C/min. Ukupholisa ngokukhawuleza kubangela i-CTE-mismatch warpage kunye ne-latent delamination. Eli nqanaba alinakukhawuleziswa.
Ukulinganiswa kobukhulu, ukuhlolwa okubonakalayo, ukujonga ubhaliso lomaleko we-X-ray (ii-fiducials zangaphakathi mazibe ngaphakathi kwe-±0.075mm ukusuka kwiithagethi zokubhola).
4.1 Iinkcukacha zeMijikelo yoShicilelo
Isigaba 1 — Ukulayisha kunye noxinzelelo lokuqala:
Inqwaba ifakwa kwincwadi yabezindaba phakathi kweefilimu ezikhuphayo kunye neepleyiti zesibuko. Uxinzelelo lokuqala loqhagamshelwano (50–100 PSI) lufakwa ngaphambi kokuba kuqaliswe ukufudumeza ukuthintela ukutshintsha komaleko ngexesha lokunyuka kobushushu bokuqala.
Isigaba sesi-2 — Irempu yobushushu (imizuzu engama-60–90):
Lawula izinga lobushushu kunye nobushushu bokuphola usebenzisa isikhokelo sokucubungula somthengisi we-laminate kunye noqwalaselo oluqinisekisiweyo lwephaneli/ukucinezela. Ubushushu obunye be-FR-4 okanye uluhlu lwezinga lokuphola alugubungeli zonke iinkqubo ze-resin kunye ne-stackup. I-ramp efanelekileyo kufuneka ixhase:
- Iyakhupha umswakama oseleyo ngaphambi kokuba i-resin ihambe
- Ivumela i-resin ukuba ifikelele kubushushu bayo bokuhamba (130–150°C) ngokulinganayo kuyo yonke iphaneli ngaphambi kokuba i-gelation epheleleyo iqale
- Inciphisa i-thermal gradient kuyo yonke iphaneli — kubaluleke kakhulu kwiiphaneli ezinkulu apho umahluko phakathi kobushushu nomphetho nombindi unokubangela ukuphiliswa okungafaniyo ukuba ukhawuleziswa ngokukhawuleza kakhulu
Isigaba sesi-3 — Uxinzelelo olupheleleyo kunye nokuphiliswa koxinzelelo (imizuzu engama-90–180):
Faka iprofayili yoxinzelelo kunye ne-live efanelekileyo kwinkqubo ye-resin, ukusasazwa kobhedu kunye nokwakhiwa kwe-press. Qinisekisa ukuba ukuhamba kwe-resin, ukubopha kunye nokulungisa kuyahlangabezana nemigangatho yenkqubo echaziweyo. Ukulinganiswa kwe-Tg okanye ukulungisa kunokuxhasa ukuqinisekiswa kwenkqubo, kodwa uxinzelelo oluqhelekileyo okanye ubushushu bodwa abumiseli umjikelo ochanekileyo.
Isigaba sesi-4 — Ulawulo lokuphola:
Sebenzisa iprofayili yokupholisa eqinisekisiweyo kwisimo sezinto kwaye ucinezele. Iigradients zobushushu kunye nokungafani kokwandiswa kunokubangela uxinzelelo olushiyekileyo kunye notshintsho lobukhulu. Ukupholisa okukhawulezayo okanye okungalinganiyo kunokubangela:
- Iphepha lokujika elikhawulezileyo (intloko ebonakalayo kunye nokujika okugqithileyo IPC-6012 imida ye-±0.75%)
- Uxinzelelo lwangaphakathi olubonakala njengokwahlukana okufihlakeleyo phantsi komjikelo wobushushu olandelayo
- Ukuqhekeka kancinci kwiindawo zokungena ngokusebenzisa ukugrumba ngexesha lemisebenzi yokugrumba elandelayo
Isigaba sokuphola sesona sinyathelo senkqubo esifutshane kakhulu kwimveliso ye-HDI engabizi kakhulu - kwaye sisona sizathu siqhelekileyo sokusilela kwe-warpage kunye nokuthembeka kwiibhodi ezenziwe phantsi koxinzelelo lweendleko.
4.2 Ukuvula okuninzi ngokuchasene nokuvula okukodwa
Iimashini zokushicilela ezininzi zicubungula ii-panel stacks ezininzi ngaxeshanye (ngesiqhelo ii-8-12 doors), apho i-door nganye ibamba i-panels enye okanye ezingaphezulu ezahlulwe zii-mirror plates. Oku kwandisa i-output ngaphandle kokutshintsha ixesha ngomjikelo ngamnye.
Ii-vacuum press ezivula kanye zisetyenziselwa oku kulandelayo:
- I-HDI eyinkimbinkimbi kakhulu ene-stackups ezingafaniyo apho ukusasazwa koxinzelelo olufanayo kubalulekile
- Ukulungiselela ukwakheka okuncinci (ngaphantsi kwe-60µm) apho kufuneka khona i-vacuum ukuthintela ukwakheka kwe-void
- Izixhobo ezisekelwe kwi-PTFE apho iiprofayili zobushushu kunye noxinzelelo zahlukile kwi-FR-4 kwaye ungcoliseko oluphakathi kwemithwalo yokushicilela luyinto exhalabisayo
Kwi-PTFE okanye i-laminate ephezulu egcwele i-ceramic, imigca yokushicilela kufuneka inikezelwe okanye icocwe kakuhle phakathi kokusetyenziswa kwezinto ze-FR-4 kunye ne-HF. Ungcoliseko olunqamlezileyo lwezinto ze-PTFE ezine-resin ye-FR-4 lutshintsha i-dielectric constant kwaye kunzima ukuyifumana ngaphandle kohlalutyo olutshabalalisayo.
4.3 Ulawulo lweNkqubo kunye nokuBeka iliso
Ukufakelwa kwe-lamination kwimveliso kwiifektri ze-HDI ezisemgangathweni kubandakanya:
Ukubeka iliso kwi-thermocouple: Ii-thermocouple ezininzi ezibekwe kwincwadi yeendaba kwiikona zephaneli naphakathi. Iimikhondo zobushushu ziyabhalwa kuyo yonke imijikelo kwaye zijongwa ngokuchasene nefestile yeprofayili yeendaba eqinisekisiweyo. Naliphi na iphaneli apho i-thermocouple iwele khona ngaphandle kwefestile yeprofayili iphawulwe ukuze kuqinisekiswe ubukhulu kunye nobubanzi.
Iikhuphoni zokuhamba kweresin: Iikhuphoni ezincinci zovavanyo ezibekwe emaphethelweni ephaneli ziqokelela ukuhamba kweresin ngexesha lokulamina. Ukuhamba kweresin ngaphandle kwefestile eyamkelekileyo (incinci kakhulu = imingxuma, ininzi kakhulu = ukususwa komphetho) kubangela uphando lomxholo womswakama we-prepreg kunye nokulinganiswa kobushushu obucinezelweyo.
Ukulinganiswa kobukhulu bephaneli: Ubukhulu be-post-lamination bulinganiswa ngama-9+ amanqaku ngephaneli nganye. Utshintsho oludlula ±10% yophononongo lwe-nominal triggers lokusasazwa koxinzelelo olungalinganiyo okanye utshintsho lwe-prepreg lot.
5. Ukucubungula iiBhayisikile eziPhakathi: Ukuhlolwa, ukuBhoboza, kunye nokuPlata phakathi kweeBhayisikile
5.1 Ukuhlolwa Emva Kokugquma Ngaphambi Komjikelo Olandelayo
Yonke imijikelo kufuneka iphumelele uhlolo ngaphambi kokuba umsebenzi uqhubekele kumjikelo olandelayo. Ukukhulula iphaneli enesiphako kumjikelo olandelayo yeyona nto ibiza kakhulu ekuvelisweni kwe-HDI — isiphako siyafihlwa, amanyathelo enkqubo ongezelelweyo asetyenziswa kwisiseko esinesiphako, kwaye ekugqibeleni iphaneli iyasuswa kuhlolo lokugqibela.
Uluhlu lokuhlola phakathi kwemijikelo:
- Ukubhaliswa komaleko we-X-reyi: ii-fiducials zomaleko wangaphakathi kufuneka zilungelelaniswe ngaphakathi kwe-±0.075mm yeethagethi zokubhola
- Ukujonga ubukhulu bephaneli: ubude, ububanzi, kunye nobukhulu ngaphakathi kweenkcukacha
- Ukuhlolwa okubonakalayo kweeblister ze-delamination, i-edge delamination, kunye ne-surface voids
- Isampulu yecandelo elinqamlezileyo (etshabalalisayo, ekwi-process coupon): i-resin void check, i-copper-resin interface ingqibelelo, uqikelelo lwamandla e-peel
5.2 Ukubhola ngeLaser Emva komjikelo ngamnye wokwakha
Ukubhola nge-laser kulandela ukwakheka kwe-lamination yangaphandle. Iiparamitha eziphambili zenkqubo:
I-CO₂ laser yokwakheka okuqhelekileyo kwe-FR-4:
- Ubude beWave: 10.6µm — ifunxwe kakuhle yi-organic resin, ifunxwe kakubi yi-copper
- Inyathelo lokutsalwa kobhedu: ukutshaya kokuqala okufutshane kuvula "ifestile" kwifoyile yobhedu engaphandle
- Ukususwa kwe-dielectric: ii-pulses ezilandelayo zisusa izinto ezilungiselelwe kwangaphambili ziye kwi-capture pad kumaleko wangaphakathi
- Ubuncinane nge-diameter: 0.10mm igqityiwe (0.12mm igrunjiwe ngaphambi kokuba iplatiwe)
- Umlinganiselo ophezulu womda: 1:1 (ubunzulu bulingana okanye bungaphantsi kobubanzi)
I-laser ye-UV (Nd:YAG) yeefilimu ezincinci kunye ne-PTFE:
- Ubude beWave: 355nm — ukususwa kwe-ablation ebandayo ngaphandle kokutsha
- Isetyenziselwa: prepreg ngaphantsi kwe-40µm, izinto eziguquguqukayo ze-polyimide, iifilimu zokwakheka ezisekwe kwi-PTFE
- Ixabiso eliphezulu nge-via ($0.015–0.040) xa kuthelekiswa ne-CO₂ (~$0.008–$0.025/nge-via, isalathiso)
- Ingcono ngomgangatho wodonga — intsalela encinci, ukususwa okucocekileyo
Indlela yokusebenzisa imaski esesikweni: Indlela eqhelekileyo yokusebenzisa i-laser ye-CO₂ apho i-foil yobhedu yangaphandle ikrolwa ngeefestile kwindawo engaboniyo ngaphambi kokuba kugqojwe nge-laser. I-laser ye-CO₂ emva koko igqobhoza nge-dielectric kwifestile evuliweyo ngaphandle kokufuna ukungena kwi-copper. Oku kunciphisa inani lee-laser pulses nge-via kwaye kuphucula ukuqina kodonga.
5.3 I-Desmear kunye neCopper engena-Electro: Ngokulungiswa kodonga
Emva kokubhola nge-laser, ngokusebenzisa iindonga kukho intsalela evela kwinkqubo yokukhupha:
- I-resin ekhabhoni (i-drill smear) evela kwi-CO₂ laser ablation
- Intsalela yefayibha yeglasi evela kwi-prepreg substrate
- Ubhedu oluxidizisiweyo kwi-capture pad
Inkqubo yokukhupha i-manganese engapheliyo:
- Isixhobo sokudumba: sidumba i-drill smear ukuphucula ukufikelela kwiikhemikhali
- I-Permanganate etch: i-oxidize kwaye isuse i-carbonized resin kunye ne-smear
- I-Reducer: inciphisa i-permanganate eseleyo kwaye isusa nayiphi na i-oxidation kwi-capture pad copper
Kwi-PTFE laminates, i-CF₄/O₂ plasma ithatha indawo ye-permanganate. I-plasma isusa intsalela yekhabhoni ngaphandle kokuhlasela i-PTFE matrix. Kufuneka amagumbi e-plasma azinikeleyo — Ungcoliseko lwe-PTFE kwimigca ye-permanganate eqhelekileyo lubangela ukungaphumeleli kokunamathela.
Emva kwe-desmear, i-palladium catalyst ifakwa kuzo zonke iindawo kuquka neendonga, kwaye i-electroless copper (0.5–1.5µm) ifakwa ukuze kwenziwe umaleko wembewu oqhubayo wokufaka i-electroplating.
ℹ Staggered vs. Stacked: Ukhetho loYilo oluMisela iindleko zokuzalisa
Ii-microvia ezihlanganisiweyo zifuna isakhiwo esifanelekileyo sokudibanisa kwaye zihlala zisebenzisa ii-microvia ezingaphantsi ezizaliswe yithusi kunye nomphezulu olungiselelwe ngokufanelekileyo. Ukuzaliswa kwe-resin kwii-via ezigrunjwe ngoomatshini okanye ngokusebenzisa ii-vias yinkqubo eyahlukileyo. Ukuxakeka kunokwenza kube lula ukwakha, kodwa akususi ngokubanzi iimfuno zokuzalisa, ukucwangcisa okanye iziqinisekiso; kuvavanya i-geometry echanekileyo kunye nendlela yokuvelisa.
5.4 Ngokuzalisa kunye nokuCwangcisa ii-Stacked Designs
Kwimizobo esebenzisa ii-stacked vias (apho i-L1–L2 via ingaphezulu kwe-L2–L3 via), i-L2–L3 via kufuneka izaliswe kwaye icwangciswe ngaphambi kokuba i-lamination yomaleko wokwakha we-L1–L2 iqhubeke:
Ukuzaliswa kweresin:
- I-inki ye-epoxy okanye ye-polymer resin ifakwe kwi-via barrel phantsi kwe-vacuum okanye i-squeegee application
- Ukuzaliswa kufuneka kugqitywe nge-95% nangaphezulu kungabikho zikhewu — izikhewu zibangela ukuphuma kwegesi ngexesha lokudibana kwakhona
- Ukunyanga kwi-150-175 ° C kwi-60-90 imizuzu
Ukucwangcisa:
- Umphezulu ozalisiweyo unokuba nedomeyini encinci (uzalise ngaphezulu) okanye uvalwe (uzalise ngaphantsi)
- Ukucwangcisa ngoomatshini (ukugquma ngebhanti okanye ukugaywa okujikelezayo) kususa izinto de umphezulu we-via ube kumgangatho ofanayo nobhedu olujikelezileyo ngaphakathi kwe-±15µm.
- Olu luhlu lubaluleke kakhulu kwi-lamination elandelayo ukuze kufunyanwe uxinzelelo olufanayo kunye nobukhulu be-bondline.
Impembelelo yeendleko: I-Fill yongeza i-$0.05–$0.15/nge, i-planarization yongeza i-$1.50–$5.00/ngephaneli. Kwi-600-via design, i-fill kunye ne-planarization kunye zinokongeza malunga ne-$31.50–$95.00/ngebhodi (uluhlu lwesalathiso — ixabiso lokwenyani lixhomekeke kwi-via count, izinto, kunye nomthengisi). Yingakho i-staggered via design — esusa omabini la manyathelo — inempembelelo enkulu yeendleko. Jonga isikhokelo seendleko se-blind bided via PCB ukuze ufumane uthelekiso olupheleleyo lweendleko ze-via architecture.
6. Iziphene eziqhelekileyo zeLamination, Izizathu ezisisiseko, kunye noThintelo
⚠ Eyona Modi iQhelekileyo yoKusilela kwe-HDI Lamination
Ukulungiswa komphezulu ongaphakathi kufuneka kubonelele ngokubopha okuthembekileyo kwinkqubo ekhethiweyo ye-resin kunye ne-copper. Ungcoliseko okanye unyango olungafanelekanga lunokubangela ukwahlukana, kodwa akukho pesenti imiselweyo yokusilela okanye umda woburhabaxa osebenzayo kuyo yonke into yokwakha. Sebenzisa ulwalathiso lomthengisi wezinto kunye nenkqubo yokuncamathelisa efanelekileyo.
6.1 Ukwahlulahlula
Inkcazo: Ukwahlukana phakathi komaleko wobhedu kunye ne-resin/iglasi laminate ekufutshane. Isenokubonakala njenge-blister okanye i-bubble kumphezulu webhodi, okanye ifihliwe kwaye ifunyanwe kuphela ngokunqamleza.
Izizathu eziphambili:
- Unyango lwe-oxide olunganelanga: amandla e-copper-resin peel angaphantsi kwe-4 N/cm ubuncinane
- Ukulungiselela ukufuma okungaphezulu kwe-0.2%: ukuveliswa komphunga ngexesha lokulungiswa kudala izithuba ezikhula zibe ziindawo zokuhlukanisa
- Unyango alwanelanga: i-resin edityaniswe ngokuyinxenye inamandla anciphileyo okubambisana
- Ungcoliseko kumphezulu wobhedu ngaphambi kokulamina
Ukuthintela: Isiqinisekiso sonyango lomphezulu wekopolo (uvavanyo lwanyanga zonke lwamandla okuxobuka kwiikhuphoni zemveliso), ukujonga ukufuma kwangaphambili kunye nokubhaka okunyanzelekileyo kwezinto ezingathobeliyo, ukucubungula iisampulu zekhuphoni emva kweloti nganye yelamination.
6.2 Iimpazamo zoBhaliso
Inkcazo: Iithagethi zokubhola kunye nee-inner layer pads azilungelelananga kakuhle, nto leyo ebangela ukuba i-annular ring inciphe okanye ingabikho xa ingabonakali nge-capture pads.
Izizathu eziphambili:
- Utshintsho lobukhulu bephaneli ngexesha lokulamina: I-FR-4 ikhula kancinci nge-XY ngexesha lokulungiswa (ngesiqhelo yi-0.02–0.05%). Iinkqubo zokubhola kufuneka zihlawulwe ngenxa yolu lwandiso luqikelelweyo.
- Ukungazinzi kobukhulu beleya yangaphakathi: iileya zangaphakathi ezingakrolwanga ngokulinganayo (ubuninzi bekopolo obuhlukeneyo phezulu vs. ezantsi) zijika ngexesha lokulayita, zisusa iimpawu kwiindawo zazo eziqhelekileyo
- Ukungalingani kwe-press stack: ii-pin zokubhalisa kufuneka zihlale ngokuchanekileyo; ii-pin ezingahlali kakuhle zivumela ukutshintsha kwe-layer
Ukuthintela: Ukulinganisa ubhaliso lwe-X-ray drill kwiphaneli nganye ngaphambi kokugrumba (kungekhona ngokwesampulu). Imbuyekezo yokulinganisa umsebenzi wobugcisa isetyenziswa kumaleko ngamnye ngokusekelwe kwiimpawu zokwandiswa kwezinto ezilinganisiweyo. Uhlalutyo lokusasazwa kobhedu ngexesha le-DFM yomaleko wangaphakathi ukubonisa uyilo olungafaniyo ngaphambi kokuveliswa.
6.3 Izinto ezingasasebenziyo kunye nokubanjwa komoya
Inkcazo: Iipokotho zomoya okanye zegesi kwi-resin ecociweyo, ezibonakala njengezinto ezifana ne-delamination okanye i-pinpoint voids kwindawo enqamlezileyo.
Izizathu eziphambili:
- Lungiselela kwangaphambili umxholo we-resin owaneleyo kuyilo lwephaneli olunikiweyo (umlinganiselo ophezulu wendawo ye-copper-to-dielectric ufuna ukuhamba kwe-resin okuphezulu)
- Ukungasebenzi kakuhle kwe-vacuum kwimijikelo yokushicilela encedisa i-vacuum
- Irempu yokuqala ekhawulezayo kakhulu ethintela ukuhamba kakuhle kwe-resin kunye nokuphuma kwegesi ngaphambi kokuba i-gel iphume
Ukuthintela: Iinkcukacha zomxholo we-resin ezihambelana noxinano lwephaneli yobhedu. I-vacuum lamination yoyilo oluneepateni zobhedu oluxineneyo. Iiprotokholi zesantya sokuhamba eziqinisekisiweyo eziqinisekisa ukuphuma ngokupheleleyo kwegesi ngaphambi kokuba kusetyenziswe iijeli ze-resin.
6.4 I-Warpage kunye neBow
Inkcazo: Ukuphambuka kwimilo yephaneli kudlula imida ye-IPC-6012 (ukugoba kunye nokujika ≤0.75% yephaneli ethe tyaba kwi-HDI Class 3, ≤1.5% kwi-Class 2).
Izizathu eziphambili:
- Ukusasazwa kobhedu olungenamlinganiselo: ukuba isiqingatha esiphezulu se-stackup sine-copper engaphezulu kakhulu kunesiqingatha esisezantsi, i-CTE eyahlukileyo ngexesha lokuphola ibangela ukugoba kwicala elinobhedu olunzima.
- Ukuphola ngokukhawuleza: i-gradient yobushushu ukusuka kumphezulu ukuya embindini weepaneli ezixineneyo ngexesha lokuphola ngokukhawuleza ivelisa amaxesha okugoba
- I-prepreg engangqinelaniyo kunye ne-core CTE: izixhobo ezahlukeneyo kwi-stackup ene-CTE ezahlukeneyo zenza uxinzelelo lwangaphakathi
Ukuthintela: Uhlalutyo lwebhalansi yekopolo ngexesha le-DFM — uxinano lwekopolo kwisiqingatha esiphezulu nesezantsi se-stackup kufuneka lube ngaphakathi kwe-±10% enye kwenye kwi-symmetric designs. Ulawulo lokubeka esweni izinga lokuphola. Kwi-designs ezingafaniyo (ezingenakuphepheka kwezinye iinkqubo), iimpawu zekopolo zekopolo ezingasemva zingongezwa ukulinganisela i-stackup.
6.5 Ukwahluka koKutyeba
Inkcazo: Ubukhulu be-dielectric emva kwe-lamination ngaphandle kwe-±10% yenkcazo, nto leyo ebangela ukuba ubukhulu be-impedance trace trace buphoswe ziithagethi zabo.
Izizathu eziphambili:
- Ukuhamba kweresin okungafanelaniyo: ukuhamba kakhulu kwimiphetho yephaneli (embindini obhityileyo), kuncinci kakhulu (imiphetho etyebileyo) — okubangelwa kukungangqinelani komxholo weresin
- Uxinzelelo lwe-press alufani kwiiphaneli ezinkulu
- Ukwahluka kwenani le-prepreg kumxholo we-resin
Ukuthintela: Ukulinganisa ubukhulu obuyi-9-point emva komjikelo ngamnye we-lamination. Ukulinganisa umxholo we-resin kwi-prepreg engenayo (hayi nje i-Dk kunye ne-Df). Ukuqinisekiswa kokuthamba kweplate yesipili (iipleyiti zesipili ezigoba emva kokuguguleka zizisa uxinzelelo olungalinganiyo).
7. Inkqubo ye-Highleap's Controlled Lamination ye-HDI PCBs
7.1 Izixhobo kunye neZiseko zeNkqubo
Ubuchule be-lamination ye-HDI ye-Highleap buquka:
- Iimashini zokushicilela ze-hydraulic ezivula ngeendlela ezininzi ezisebenzisa i-vacuum kunye nobushushu obufanayo be-±1°C kwi-press platen
- Imigca yokushicilela ye-PTFE/specialty low-loss families laminate ezinikeleyo — akukho kungcoliswa okunqamlezileyo kwimigca yokushicilela ye-FR-4
- Ukugcinwa kwangaphambili okulawulwa yimozulu kwi-≤21°C, ≤45% RH kunye nokujonga ukufuma nge-lot nganye
- Ukungena kwi-thermocouple kwi-intanethi kuyo yonke imijikelo yemveliso ye-lamination
- Ukulinganiswa kobhaliso lwe-X-reyi kwi-100% yeepaneli (hayi iisampulu) ngaphambi nasemva kokubhola nge-laser
7.2 Iprotocol yoHlolo lweeMijikelo ezahlukeneyo
Phakathi komjikelo ngamnye we-lamination, iHighleap iqhuba:
- Ukuhlolwa kobhaliso lwe-X-ray eyi-100%: zonke ii-fiducials ze-inside layer zilinganisiwe, azithathwanga isampuli
- Ukumapha kobukhulu bephaneli kwiindawo ezili-9: nayiphi na iphaneli engaphandle kwe-±10% isusiwe kwimveliso
- Ukuhlolwa okubonakalayo kweeblister ze-delamination kunye nokwahlukana komphetho
- Icandelo lekhuphoni yenkqubo (ikhuphoni enye ngeqela lemveliso): umlinganiselo wamandla okuxobula, ukujonga i-resin void, uvavanyo lomgangatho womdibaniso we-copper-resin
Le geti yemijikelo ephakathi ibamba ama-85–90% eziphene ze-lamination ngaphambi kokuba kusetyenziswe utyalo-mali olongezelelweyo lwenkqubo kwiphaneli echaphazelekileyo. Ixabiso lokubamba isiphene kuhlolo lwemijikelo ephakathi xa kuthelekiswa novavanyo lokugqibela lombane: malunga ne-$15 xa kuthelekiswa ne-$85 kwiindleko zenkqubo echithiweyo (amanani abonisayo). Ukuze ufumane impembelelo yeendleko zesivuno kunye nokubalwa komjikelo we-lamination, jonga i-blind waved nge-PCB cost analysis . Ukuze ufumane impembelelo yexesha lomjikelo ngamnye we-lamination, jonga isikhokelo sexesha lokhokelo lwe-HDI PCB.
7.3 Ukuphathwa kwezinto kunye nokulandelelwa kweLoti
Yonke indawo yemveliso ibandakanya ukulandeleka okugcweleyo kwezinto: inombolo ye-prepreg lot, i-copper foil lot, kunye ne-laminate core lot — zonke zidibene neerekhodi zomhambi wemveliso kunye nokuhlolwa. Kwiinkqubo ze-controlled-impedance, i-prepreg Dr ilinganiswa kwiikhuphoni ze-lot engenayo kwaye ixabiso elilinganisiweyo lisetyenziselwa ukubala i-impedance yokugqibela (hayi ixabiso le-datasheet elimiselweyo), ukuqinisekisa ukuba iziphumo zekhuphoni ze-TDR ziyaphindaphindeka ukusuka kwi-lot ukuya kwi-lot (jonga iimfuno ze-PCB ze-impedance ezilawulwayo )
7.4 IiMetriki zoMgangatho we-HDI Lamination eHighleap
- Uhlobo I HDI lamination yield (iphaneli ephumelele zonke ii-inter-cycle auditions): 97.8% avareji
- Uhlobo lwesibini lwe-HDI lamination isivuno: 95.2% avareji
- Uhlobo lwesithathu lwe-HDI lamination isivuno: 91.6% avareji
- Izinga lokususwa kwe-delamination ekuhlolweni kokugqibela: ngaphantsi kwe-0.3% yeepaneli ezithunyelweyo
- I-impedance elawulwayo yokuqala isivuno (ngaphakathi kwe-±10%): 98.1% yezabelo
- Ukuthobela i-Warpage (ukugoba kunye nokujika ngaphakathi kwe-spec): 99.2% yeephaneli ze-HDI
Ezi milinganiselo ziyafumaneka xa ziceliwe ngeenjongo zokufaneleka komthengisi.
Izithuba kucetyiswa
Ukwenziwa kwe-TMM PCB
Isiqulatho I-TMM PCB Fabrication Scope ye-RF kunye...
RT duroid 6002 PCB Quote kunye Stackup
Eli phepha liphethe umsebenzi wesicatshulwa kunye nenkcazo ye-stackup...
Ukuveliswa kwePCB yesihluzo se-TMM6
Uluhlu lweziqulathoKutheni Abayili beeMicrowave Filter beSebenzisa...
I-Taconic RF 35 vs RO4350B PCB
Uluhlu lweziqulathoRF-35 vs RO4350B Ukuthengwa kunye...
Indlela yokufumana isicatshulwa kwiiPCBs
Masikwenzele uhlalutyo lweDFM/DFA kwaye sibuyele kuwe ngengxelo.
Ungalayisha iifayile zakho ngokukhuselekileyo kwiwebhusayithi yethu.
Sifuna olu lwazi lulandelayo ukuze sikunike ikowuti:
-
- Gerber, ODB++, okanye .pcb, spec.
- Uluhlu lwe-BOM ukuba ufuna ukudibanisa
- ubuninzi
- Ixesha lokujika